Warping is the oldest problem in FDM printing and it still catches people out, partly because the advice for it is usually written for the easy case: a wide, flat part in ABS, fixed with a hotter bed and an enclosure. The case I actually have in front of me is different. I have a part with a thin base and tall, thin sides, and the sides are pulling the base up off the plate. That is a geometry problem more than a settings problem, and most general guides barely touch it. So this post covers the full set of warping fixes, then goes specifically at that thin-base, tall-wall situation, which turns out to be a well-recognised one with some genuinely useful design answers.
Why prints warp
Every thermoplastic shrinks as it cools from melt temperature back to room temperature. Warping is what happens when that shrinkage is uneven or restrained. The layers closest to the plate are held in place by the bed, so they cannot shrink freely, and the stress builds up inside the part instead. Corners go first because that is where two directions of shrinkage meet and there is the least material holding them down. When the stored stress exceeds the grip of the first layer, the edges peel upwards. The more a material shrinks, the worse it gets: PLA barely warps, PETG is mild, and ABS, ASA, nylon and polycarbonate are the notorious ones, as the PLA, PETG and nylon posts explain.
Reading when it happens
The timing of the lift tells you a great deal, and it is the first thing to look at.
| When it lifts | Likely cause | Where to start |
|---|---|---|
| Within the first 10 to 20 layers | A dirty plate, a cool bed, a first layer that never bonded, or the part fan starting too early | The first layer troubleshooting post and the bed adhesion post |
| Only after the print gets tall | Accumulated shrinkage stress, or ambient air that is too cold | Design changes, warmer surroundings, brim |
| One side lifts and the other holds | A draft, uneven bed heating, or a warped plate | Move away from vents, check the plate is flat |
| The whole part detaches and gets dragged | The first layer never adhered | Reset first-layer height and clean the plate |
| Base stays flat but the part bows in the middle | Shrinkage in a large flat plate-like model | Ribs, splitting the part, or reorienting it |
A thin base with tall sides sits in the second row. It rarely fails in the first few layers, because the first layer is fine. It fails as the walls grow, which is the signature of accumulated stress rather than a bad start.
The thin base, tall walls problem
Here is the mechanism in plain terms, with the caveat that this is reasoning from the general explanation rather than a measurement. Each new layer of wall is laid down hot onto cooler plastic beneath, then shrinks as it cools, and because the layers are bonded together that pull accumulates up the height of the wall. A tall wall behaves like a long strip of material trying to contract, and the only thing resisting it at the bottom is the base. If the base is thin, it has very little stiffness to resist bending, so instead of holding flat it gets pulled inwards and upwards at the edges. The taller the walls, the greater the accumulated pull. That matches what the guides say: corners that lift only after the print gets tall point to built-up shrinkage stress, and thin tall walls are described as vulnerable because they have little cross-section to resist bending. Stratasys Direct, quoted in one summary, warns that large extents of minimum-thickness vertical walls can warp unless ribs or a support tower are used.
One more subtlety is worth knowing, from forum threads on exactly this kind of print. The part can stay stuck to the plate on all sides, and the magnetic build sheet itself lifts at the edges, giving the same warped result. Strong adhesion is not always the answer, because past a point you are asking the sheet to resist the stress, and it can lose to the magnets. Check whether the part is peeling off the sheet or the sheet is peeling off the bed, because the two need different responses. It is also worth checking that nothing is trapped under the sheet, as covered in the first layer rippling post.
Fix the design first: it works better than any setting
Several sources make the same point forcefully: warping is often more a design issue than a printer issue, and a design change reduces stress far more reliably than a brim. If you can edit the model, or ask the designer to, these are the changes that help most.
| Design change | What it does | Notes |
|---|---|---|
| Round the corners and add fillets or chamfers at the base | Stops stress concentrating at a sharp point | Rounded corners warp far less because the peeling force cannot focus on one spot |
| Thicken the base | Gives the base more stiffness to resist being pulled | The most direct answer to a thin base, if the function allows it |
| Add ribs, gussets or a support tower between base and walls | Stiffens the junction so the base cannot bow | Recommended for large runs of thin vertical wall; adds material, so test it |
| Break up continuous walls | Interrupts the path along which stress accumulates | Gaps, slots or relief cuts in a long wall reduce the pull; a designer’s tip from the MakerWorld community |
| Break up large flat areas on the base | Small grooves or cutouts stop one big plane pulling as a unit | Helps when the base is wide as well as thin |
| Make transitions gradual | Avoids abrupt thick-to-thin changes that build pulling forces | A model that widens sharply above a narrow base is especially prone |
| Split the part and join it afterwards | Turns one high-stress part into several low-stress ones | The multi-part printing post covers splitting and joining |
| Reorient the part | Changes which faces are on the plate and how the stress builds | Tall thin parts are reported to warp less at around 45 degrees, though this may need supports |
One trade-off deserves flagging, because the advice is contradictory on purpose. More walls and higher infill density resist shrinkage somewhat, but more plastic also means more force when it does shrink. One forum reply on a warping base plate suggests thin walls and sparse infill can make a print more flexible and prone to distortion, while the same reply notes that extra material may increase the pulling force. A MakerWorld designer reports success using gyroid infill to reduce the pulling forces on the outer walls, though that is one person’s experience. The infill patterns post covers why gyroid behaves well. The honest advice is to test rather than assume, changing one thing at a time.
Anchor it: brim and mouse ears
A brim is the highest-value change you can make on a warp-prone print, because it adds grip exactly where lifting starts. The guides suggest 5 to 10mm, with a Bambu-specific guide recommending an outer brim of around 8mm, and a wider one for stubborn cases. If only the corners lift, mouse ears do the same job with far less cleanup. The skirt, brim and raft post covers the settings. Two cautions from the sources are worth keeping in mind. A forum reply on a lifting ASA print suggests setting the brim-to-part gap to zero rather than a small gap, so the brim is truly attached. And a very wide brim can warp at its own outer edge, behaving like a thin flat part and pulling the corner up with it, so wider is not always better.
Control the heat: bed, fans and surroundings
| Material | Warp risk | Bed temperature to aim for | Part fan | Enclosure |
|---|---|---|---|---|
| PLA | Low | About 60 to 65°C, never above 65 | Off or low for early layers, then as normal | Not needed, and can be counterproductive |
| PETG | Low to moderate | About 70 to 85°C | Low, roughly 30 to 50% | Not needed, but no drafts |
| ABS / ASA | High | About 95 to 110°C | Off to very low | Essentially required |
| Nylon / PC | High | About 100°C or more | Off | Required, and warmer than for ABS |
Several points sit behind that table. Raising the bed by about 5°C toward the top of the material’s range keeps the bottom layers warmer for longer, so they stiffen later and pull less. Keep the part cooling fan off or low for the first layers, and consider reducing it further for thin tall walls, since walls that curl near the top can mean cooling that is too strong, which a minimum layer time setting can also help with. Bambu’s own guidance on warping highlights the auxiliary fan as the cause most people miss, since it blows air across the part and chills one side. And drafts matter: close windows and doors and keep the printer away from vents, as one side cooling faster than the other is a classic cause of one-sided lifting.
On enclosures, the advice depends on material and is worth getting right. For ABS and ASA an enclosure is the real fix, and everything else is a workaround. For PLA it is not just unnecessary but potentially harmful: PLA’s glass transition is around 60°C, and a warm enclosed chamber can soften tall thin walls into sagging and contribute to the heat creep covered in the heat creep post. That is relevant to the open-frame A1 and A2L, where Bambu itself does not recommend enclosing the A1, as the A1 enclosure post explains. If you are printing a warp-prone material on an open machine, switching to a lower-shrink material is usually wiser than building a box.
A forum thread on a lifting ASA box adds a few thermal tips that are worth trying on any material prone to this: lower the nozzle temperature after the first layer, raise the bed temperature slightly (but not too far, or you invite elephant’s foot, covered in the elephant’s foot post), pre-heat the chamber before starting, and reduce layer height so less heat is added per layer. Treat these as experiments rather than guarantees.
Don’t forget the basics
Before spending effort on advanced fixes, make sure the first layer is actually good. The common culprits are fingerprint oil on the plate, a Z offset that is too high, a first layer printed too fast, a cool bed, and the fan starting before the base has bonded. Wash the plate, confirm the first layer is smooth and fused, and check for rippling or debris as covered in the first layer rippling post. A marginal first layer can survive a small part and fail on a tall one, so tall prints are the ones that expose it.
A word on adhesives: glue stick and hairspray can help warp-prone materials like ABS and ASA on glass or smooth plates, but on PLA on a clean PEI sheet they tend to reduce grip, as the bed adhesion post explains, so do not reach for glue by reflex.
A plan for a thin base with tall thin sides
- Diagnose which thing is lifting. Watch a print, or check afterwards: is the part peeling off the sheet, or is the sheet lifting off the bed? Rule out debris under the sheet.
- Get the first layer genuinely good. Clean plate, correct plate selected, smooth and fused lines, first-layer fan off.
- Change the design if you can. Thicken the base, add fillets and rounded corners, add ribs or gussets at the base-wall junction, or break up the long walls with relief cuts or slots.
- Add a brim or mouse ears. Start around 8mm with the brim gap at zero, using mouse ears if only corners lift.
- Warm the bed to the top of its range for the material, and cut the part and auxiliary fan during the early layers, reducing them for the thin walls.
- Remove drafts. Close doors and windows and move the printer away from vents.
- Try reorienting. Tilting the part, if supports are acceptable, changes how the stress builds.
- Consider splitting the part, printing the base and walls separately and joining them, if the function allows.
- Consider a lower-shrink material, such as PLA+ or PETG, if you are fighting ABS, ASA or nylon on an open printer.
One practical tip for iterating: because the problem only appears as the walls get tall, testing with the whole model wastes hours. Cut the model in the slicer so you print only the lower portion, perhaps the first 30 to 40mm, and see whether the base stays flat, then raise the height as the fixes work. That is my suggestion rather than something from the sources, but it follows from how the failure develops.
Common mistakes
- Treating a geometry problem as a settings problem, and spending hours on temperatures when the design is the cause.
- Building an enclosure for PLA, which can soften tall thin walls and cause heat creep.
- Making the brim enormous when a moderate brim, or mouse ears, would do, and ending up with the brim itself warping.
- Pushing the bed temperature too high for PLA, above about 65°C, which makes the material soft.
- Adding glue to PLA on a clean PEI sheet and reducing grip.
- Assuming the part is peeling, when it is the magnetic sheet lifting at the edges.
- Printing the whole tall model for every test, instead of a cut-down version.
The summary
Warping is shrinkage stress beating adhesion, and the stress comes from the geometry as much as from the material. A thin base with tall thin walls is a textbook stress trap: the walls accumulate shrinkage as they grow, and the thin base cannot resist being pulled. The fixes that work best are in the design, thickening the base, rounding corners, adding ribs and breaking up long walls, followed by anchoring with a brim or mouse ears and managing heat with the right bed temperature, low fans and no drafts. Keep an enclosure for the materials that genuinely need one, and avoid it for PLA. Work through the plan in order, change one thing at a time, and test with a cut-down model so each experiment takes minutes rather than hours.